Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultramid® A3WC4 - PA66-CF20 - BASF

Material Data Center offers the following functions for Ultramid® A3WC4:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Ultramid A datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Product Texts
Electrically conductive grade reinforced with 20 % carbon fibres. Used for machinery elements and housings with high stiffness and dimension stability, low density and favourable frictional behaviour (eg connecting rods).
Processing/Physical Characteristicsdry / condUnitTest Standard
ISO Data
Melt volume-flow rate, MVR 10 / * cm³/10min ISO 1133
Temperature 275 / * °C -
Load 5 / * kg -
Mechanical propertiesdry / condUnitTest Standard
ISO Data
Tensile Modulus 17000 / 12000 MPa ISO 527
Stress at break 230 / 160 MPa ISO 527
Strain at break 2.5 / 6 % ISO 527
Tensile creep modulus, 1h * / 8000 MPa ISO 899-1
Tensile creep modulus, 1000h * / 6800 MPa ISO 899-1
Charpy impact strength, +23°C 60 / 70 kJ/m² ISO 179/1eU
Charpy impact strength, -30°C 50 / - kJ/m² ISO 179/1eU
Charpy notched impact strength, +23°C 11 / 16 kJ/m² ISO 179/1eA
Charpy notched impact strength, -30°C 7.5 / - kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
ISO Data
Melting temperature, 10°C/min 260 / * °C ISO 11357-1/-3
Temp. of deflection under load, 1.80 MPa 245 / * °C ISO 75-1/-2
Temp. of deflection under load, 0.45 MPa 250 / * °C ISO 75-1/-2
Coeff. of linear therm. expansion, parallel 9 / * E-6/K ISO 11359-1/-2
Coeff. of linear therm. expansion, normal 86 / * E-6/K ISO 11359-1/-2
Burning Behav. at 1.5 mm nom. thickn. HB / * class IEC 60695-11-10
Thickness tested 1.6 / * mm -
Yellow Card available yes / * - -
Burning Behav. at thickness h HB / * class IEC 60695-11-10
Thickness tested 0.8 / * mm -
Yellow Card available yes / * - -
Electrical propertiesdry / condUnitTest Standard
ISO Data
Volume resistivity 0.0155 / 0.014 Ohm*m IEC 62631-3-1
Surface resistivity * / 4600 Ohm IEC 62631-3-2
Electric strength 5 / 5 kV/mm IEC 60243-1
Comparative tracking index - / 100 - IEC 60112
Other propertiesdry / condUnitTest Standard
Water absorption 6.5 / * % Sim. to ISO 62
Humidity absorption 2 / * % Sim. to ISO 62
Density 1220 / - kg/m³ ISO 1183
Material specific propertiesdry / condUnitTest Standard
ISO Data
Viscosity number 150 / * cm³/g ISO 307, 1157, 1628
Test specimen productionValueUnitTest Standard
ISO Data
Injection Molding, melt temperature 290 °C ISO 294
Injection Molding, mold temperature 80 °C ISO 294
Injection Molding, injection velocity 200 mm/s ISO 294
Processing Recommendation Injection MoldingValueUnitTest Standard
Pre-drying - Temperature 80 °C -
Pre-drying - Time 4 h -
Processing humidity ≤0.15 % -
Melt temperature 280 - 300 °C -
Mold temperature 80 - 90 °C -
Diagrams
Dynamic Shear modulus-temperature , Ultramid® A3WC4 (dry), PA66-CF20, BASF
Stress-strain , Ultramid® A3WC4 (dry), PA66-CF20, BASF
Secant modulus-strain , Ultramid® A3WC4 (dry), PA66-CF20, BASF
Stress-strain (isochronous) 23°C, Ultramid® A3WC4 (cond.), PA66-CF20, BASF
Creep modulus-time 23°C, Ultramid® A3WC4 (cond.), PA66-CF20, BASF
Creep curve 23°C, Ultramid® A3WC4 (cond.), PA66-CF20, BASF
Stress-strain (isochronous) 90°C, Ultramid® A3WC4 (dry), PA66-CF20, BASF
Creep modulus-time 90°C, Ultramid® A3WC4 (dry), PA66-CF20, BASF
Creep curve 90°C, Ultramid® A3WC4 (dry), PA66-CF20, BASF
Stress-strain (isochronous) 120°C, Ultramid® A3WC4 (dry), PA66-CF20, BASF
Creep modulus-time 120°C, Ultramid® A3WC4 (dry), PA66-CF20, BASF
Creep curve 120°C, Ultramid® A3WC4 (dry), PA66-CF20, BASF
Tensile modulus-temperature , Ultramid® A3WC4 (dry), PA66-CF20, BASF
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Additives
Lubricants, Release agent
Special Characteristics
Increased electrical conductivity, Heat stabilized or stable to heat
Regional Availability
Europe
Other text information
Injection molding
PREPROCESSING
Pre/Post-processing, max. allowed water content: .15 %
Pre/Post-processing, Pre-drying, Temperature: 80 °C
Pre/Post-processing, Pre-drying, Time: 4 h

PROCESSING
injection molding, Melt temperature, range: 280 - 300 °C
injection molding, Melt temperature, recommended: 290 °C
injection molding, Mold temperature, range: 80 - 90 °C
injection molding, Mold temperature, recommended: 80 °C
injection molding, Dwell time, thermoplastics: 10 min
Chemical Media Resistance
Acids
Acetic Acid (5% by mass) (23°C)
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.